Pororsity Tests

Pororsity Tests*-150 to 200 gram Sections of fired filters were cut out of the lip, weighed, soaked for 24 hours and then re-weighed to evaluate.

Ceramic Water Filter Test Batch No. 1
Thursday January 18, 2007
Pororsity Test*- 38.8%
******

Ceramic Water Filter Test Batch No. 2
Saturday January 20th, 2007
Pororsity Test*- 32.2%
Mix Proportion represents 10% less sawdust than mix No. 1

******

Ceramic Water Filter Test Batch No. 3
January 22, 2007
Pororsity Test*- 34.5%
Mix Proportion represents 20% less sawdust than mix No. 1

******

Ceramic Water Filter Test Batch No. 4
January 24, 2007
Pororsity Test*- 45.6%
Mix Proportion represents 10% more sawdust than mix No. 1
******
Ceramic Water Filter Test Batch No. 5
January 25, 2007
Pororsity Test*- 49.7%
Mix Proportion represents 20% more sawdust than mix No. 1

Technorati Tags : ,

Ceramic Water Filter Series Batch Tests Firing

Feb 8th, 2007
20 filters in firing – Target temperature 890 C.
Gas firing

Kiln On  — 1 Burner
1:00 187 C 2 Burners
2:06 277 C 4 Burners
3:20 523 C 6 Burners
4:00 544 C
4:58 560 C
5:40 682 C
6:06 707 C
6:38 805 C
7:12 850 C
7:21 861 C
7:40 890 C Begin Soak
8:00 893C
8:21 897C
8:40 894 C
9:00 Kiln Off

Firing Descriptions:

Of 20 filters 17 cracked during the firing. These cracks appeared to be dunts due apparently to rapid firing. The firing also revealed carbon retained in the filters mostly in the bottom of the filters. Of the three filters which were not cracked, two had carbon in the bottoms. The retained carbon appears to be caused either from insufficient soaking and or the method of stacking the ware in the kiln.